FINISHED PRODUCT

Longitudinal reversion

ISO 2505:2023 · air oven method

STANDARDISED

Dimensional stability of the pipe after heat exposure.

Purpose and principle

Assess the longitudinal dimensional stability of a pipe after heat exposure. The change in distance between two marks is expressed as a percentage.

Conditions / parameters

Specimens3 sections · length 200 ± 20 mm
Initial distanceL₀ = 100 mm between marks
Conditioning23 °C · 3 h
Thermal cycle135 °C · 1 h

Test setup

Retrait longitudinal : éprouvette avant chauffage et après refroidissement.
Longitudinal reversion · distance between marks before heating and after cooling.

Test procedure

  1. Condition the pipes, cut three specimens and make two marks.
  2. Measure the distance L₀ at room temperature before heating.
  3. Heat using the specified cycle, without contact with the oven walls; allow to cool freely.
  4. Measure L after cooling, calculate the percentage for each specimen and check its appearance.

Expression / calculation

RL = 100 × (L₀ − L) / L₀   [%]
(+ = shrinkage; − = elongation)