FINISHED PRODUCT

Socket fusion welding and assembly

PP-R pipe-to-fitting assembly method · preparation, heating and joint inspection

SUPPLEMENTARY

Controlling socket fusion and checking assembly quality.

Purpose and principle

Make a PP-R pipe-to-fitting joint by heating both mating surfaces simultaneously, then joining them axially without rotation. After cooling, joint quality is assessed by visual and manual checks and, as a supplementary measure, hydrostatic testing.

Conditions / parameters

Assembly shownPP-R pipe and fitting, DN 20 (illustrated example)
ProcessSocket fusion using heating dies matched to the diameter
Parameters to controlDie temperature, heating and assembly times, insertion depth and waiting time before testing
ChecksCut and cleanliness · depth marks · bead, alignment and joint integrity

Socket fusion principle

Assemblage PP-R par polyfusion : chauffer, emboîter et contrôler.
Simultaneous heating of the surfaces · axial joining without rotation · cooling before inspection.

Operating procedure

  1. Prepare: fit the dies while the tool is cold, check its temperature, cut the pipe square and mark the insertion depth and alignment.
  2. Heat: engage the pipe and fitting simultaneously on the correctly sized dies, up to the mark, without rotation and for the specified time.
  3. Assemble: quickly remove both parts, join them axially without rotation, follow the marks and leave the joint to cool without loading.

Welding parameters — DN 20 to 63

Ø (mm)Heating (s)Assembly (s)Before operational testing (min)Pipe insertion (mm)
2054214
2574316
3286418
40126420
50186423
63248627

Reference table for socket fusion welding. Confirm the settings against the tool instructions and installation conditions; operational testing takes place after the stated waiting time.

Key process controls

Check the die temperature and observe the assembly times. Avoid rotating the parts or applying any load during cooling.